Gah! I finally get a couple hours to work on my glaze conversions, and - boom! - five formulas in, the Glazemaster software just ceases to work. So aggravating! It just keeps giving me the Hourglass of Despair. I've sent an email to the folks who sold it to me; I think I may have to de-install and re-install, with a new installation code, which I have to get from them.
Anyway! Here's what I was able to do before the derp dropped:
Recipe
Name: Magic White ^6 Test 3A
Cone:
6 Color: White
Firing:
Salt/Soda Surface: Semiglossy
Amount
Ingredient
19.5
Feldspar--Custer
6
Zinc Oxide
18
Whiting
9
Kaolin--EPK
19
Silica
15
Zircopax
4.5
Spodumene--Foote
9
Gerstley Borate--1999
100
Total
Comments:
Careful not to get it too thick! Will crawl or even split ware.
Recipe
Name: Magic White ^6 Test 4A
Cone:
6 Color: White
Firing:
Salt/Soda Surface: Semiglossy
Amount
Ingredient
18.3
Feldspar--Custer
5.6
Zinc Oxide
18.6
Whiting
8.4
Kaolin--EPK
19.4
Silica
13.9
Zircopax
4.2
Spodumene--Foote
11.6
Gerstley Borate--1999
100
Total
Recipe
Name: Tenmoku ^6 Test 1
Cone:
6 Color:
Firing:
Surface:
Amount
Ingredient
53.3
Nepheline Syenite
19.5
Silica
15.2
Whiting
7.1
Ball Clay--Old Mine #4
4.8
Lithium Carbonate
99.9
Total
Additives
7.6
Iron Oxide--Red
2.1
Bentonite
Recipe
Name: Tenmoku ^6 Test 2
Cone:
6 Color:
Firing:
Surface:
Amount
Ingredient
45.6
Nepheline Syenite
22.2
Silica
17.3
Whiting
8.1
Ball Clay--Old Mine #4
6.8
Frit--Ferro 3134
100
Total
Additives
8.7
Iron Oxide--Red
2.4
Bentonite
Recipe
Name: Satin Black ^6 test
Cone:
6 Color:
Firing:
Surface:
Amount
Ingredient
59
Albany Slip
13.5
Feldspar--Custer
4.5
Strontium Carbonate
6
Talc
15
Whiting
2
Kaolin--EPK
100
Total
Additives
1
Chromium Oxide
3
Iron Oxide--Red
2
Manganese Dioxide
1
Cobalt Carbonate
Will be mixing these up today, as well as full buckets of the successful test from last time, for the next firing - hopefully this weekend.